You’ve specified nylon, or another hygroscopic resin, and the first shots came back with silver streaks, a brittle break, or a weld that failed in your hand. Before you blame the tool or the grade, ask whether the resin was dry enough when it went into the press. This page covers resin drying and how to measure moisture in plastic resin, without treating one temperature or moisture number as a universal spec.
Generic illustration, not a part ProteForm made.
Why must nylon and other resins be dried before molding?
Many engineering plastics pick up water from the air. Nylon is the one buyers meet first, whether you specified PA6 or PA66, a copolymer, or a glass-filled nylon grade. PET and PBT behave the same way, and polycarbonate is often dried as well. The pellet looks dry. It is not necessarily dry enough to melt.
Once that moisture is in the barrel, some of it flashes to steam and leaves splay, bubbles, or a short shot. Some of it reacts with the polymer at melt temperature and cuts the chains. That second effect, hydrolysis, is why a nylon part can look almost filled and still snap in a way the datasheet never suggested. For these materials, drying is part of making the part.
The drying temperature, the time, and the moisture limit are not generic “nylon” numbers. They come from the material supplier’s datasheet for that exact grade, and they change with storage, opened bags, and regrind. This page will not invent those figures. If a quote lists a cycle, ask which datasheet it came from.
What does wet resin actually do to the part?
You’ll usually see it first as a cosmetic complaint, then as a mechanical one. Splay (silver streaks) follows flow, often worse near the gate or on a polished face. Voids, short shots, and dull or burned patches appear when steam and degraded melt disrupt filling. Weld lines become the place the part breaks. A tensile or impact test, or a simple flex in your hands, comes in below what you expected from the grade.
Not every splay mark is moisture. Trapped air, a degraded or wet colorant, or a venting problem can look similar. “Dry it longer and try again” is a weak plan if nobody has measured the resin or looked at the dryer. Moisture is a common cause on nylon, PET and PC. It is not the only cause. For a wider map of marks at the press, see injection molding defects. A part molded from wet nylon can also look acceptable on day one and still be brittle, because hydrolysis has already shortened the chains. If the duty is structural, ask for a mechanical check on T1 parts, not only a visual one.
Which resins are the ones to worry about?
Start with anything in the nylon family. Nylon 6 and nylon 66 both absorb moisture readily, and glass fiber does not cancel that. PET, PBT and polycarbonate are in the same conversation. If the datasheet has a drying section, treat drying as part of the process. Commodity polyolefins such as PP and PE pick up much less moisture, though surface water or a wet masterbatch can still mark a part. The datasheet and the lot in front of you decide.
| What you specified | Why drying comes up | What to ask, not what to invent |
|---|---|---|
| Nylon (PA6, PA66, copolymers, glass-filled) | The pellet absorbs moisture; wet melt hydrolyzes and marks the surface | Which datasheet sets the cycle and target, and whether the shop will measure moisture or only report dryer time |
| PET, PBT, polycarbonate | Hydrolysis and steam marks, or a loss of toughness | The supplier drying section, dryer type, and what happens if a bag sits open |
| A resin whose datasheet is silent on drying | Surface water or a wet additive can still mark a part | What the shop actually does with that grade, and why |
Send drawings for a nylon or resin-drying review
If the part is nylon, PET, PC or another hygroscopic grade, send the model or drawing, the exact material (or the datasheet), quantity, and the duty the part has to live in. We’ll review the design for manufacture, confirm which supplier would make it, and only then quote. We will not invent a drying temperature or a moisture limit for your grade.
How should you talk about resin drying in an RFQ?
You do not need to write a drying SOP in the RFQ. You do need to stop the shop from assuming a generic “plastic.” Name the grade, not only “nylon.” If you already have the supplier drying section, attach it. If the resin is buyer-supplied, say how it will arrive and who keeps it dry at the press. State whether regrind is allowed. Regrind has already been melted once; it can pick up moisture faster than virgin pellets. Our guide to regrind in molded parts covers how to write that note.
If appearance or a structural test is how you will accept the part, say so, so drying is treated as a process input. If you want the method recorded (dryer type, dew point if they use a desiccant system, how they measure moisture), ask for that in the process notes, not as a surprise at T1. For the rest of the pack, see what should be included in a plastic parts RFQ.
How do shops dry resin, in principle?
On a production press the usual setup is a hopper dryer on the machine, most often a desiccant dryer. Dry air is circulated through the pellets so moisture can leave the resin and not come straight back from a humid shop. The dew point of that air matters; a unit whose desiccant is spent will “dry” resin in name only. Hot-air dryers without a desiccant system are used on some jobs, and for a strongly hygroscopic resin in a humid plant they are often the wrong tool.
Tray or oven drying is still common for small lots. It can work if the batch is timed to the datasheet and then kept dry until it is molded. The equipment name matters less than whether the cycle matches the datasheet and whether the resin is still dry at the throat of the machine. Over-drying is a real risk on some grades.
How do you measure moisture in plastic resin?
Asking “did you dry it?” is not a measurement. If moisture is likely to decide T1, you want to know how the shop measures moisture in plastic resin, how often they do it, and which limit they compare the reading to. On the shop floor, the common instrument is a moisture analyzer that works by loss on drying: a small sample is heated and the weight loss is treated as moisture. It is a useful process check if the result is read against the datasheet for that grade. For a tighter reading, laboratories often use Karl Fischer titration. A supplier certificate describes the bag as shipped, not resin that sat open, was blended with regrind, or spent a weekend in a hopper that was not running.
What should you ask at T1 if the parts look wet?
If first shots show splay, unexplained short shots, or a brittle break, ask for the drying setup in writing: dryer type, dew point if they monitor it, how long that lot was in the hopper or tray, whether the bag was open, whether regrind was used, and whether anyone measured moisture, with what method, against which datasheet values. A verbal “we dried it” does not let you compare the next attempt to this one. The next shots should be tied to a stated cycle and, where it matters, a moisture reading. If the defect remains after a documented dry lot, look at venting, melt temperature, colorant, or the tool before you keep blaming the bag.
How this works if you send the job to ProteForm
We work with a network of factories in China we know well. We go through your files, tell you which factory would make it, and only then quote. If the resin is hygroscopic, that review includes whether the shop can dry and, where needed, measure that grade, not only whether they have a press the right size. We do not spray your pack across a long list of shops, and we will not invent a drying recipe. Send a model or drawing, the exact material or the requirements that force it, quantity, and the duty. If you already have a datasheet or a moisture method, attach it.
When we are not the right fit
If you need a laboratory, as a standalone service, to measure moisture in a bag of resin, or a consultant to write a drying SOP for a factory we are not coordinating, that is not our work. If you want a universal drying temperature, time, or moisture-ppm limit for “nylon” or “PC” to reuse on every drawing, we will not provide one. Those figures belong on the datasheet for the grade in front of you. If you have no drawing, no grade, and no duty, or you only want us to referee a drying dispute by email, we will decline.
What to include in an RFQ (when drying may matter)
- The model or drawing, the revision, and the exact resin grade, not only “nylon” or “plastic.”
- The material datasheet, or a link to it, if you already have the drying section.
- Whether resin is buyer-supplied or shop-purchased, how it will arrive, and whether regrind is allowed.
- The duty of the part, and whether T1 will include a mechanical or cosmetic check that moisture could affect.
- Any process note you already require, such as a recorded moisture method, without inventing a limit the datasheet does not support.
Frequently asked questions
Do I always have to dry nylon before molding?
For melt processing, treat drying as part of the process unless the grade datasheet says otherwise. A sealed bag is not a guarantee the resin is still dry at the machine, especially after it has been opened or blended with regrind.
How do I measure moisture in plastic resin?
Shops commonly use a loss-on-drying moisture analyzer as a process check. Karl Fischer titration is often used when you need a more specific water measurement. A supplier certificate describes the lot as shipped, not the hopper later. Compare any reading to the datasheet for that grade. This page will not give a universal ppm limit.
Can I put a drying temperature and time on my drawing?
You can, if those figures come from the current datasheet for your grade, or from a method you and the shop have agreed. Do not copy a cycle from a different resin or from a generic “nylon” note and treat it as a spec.
Is glass-filled nylon less sensitive to moisture?
No. The fiber does not remove the need to dry the resin. On a structural or filled part, a weak weld or a brittle break is often more obvious, not less. See the glass-filled nylon guide for what to specify besides drying.
Will ProteForm give me the moisture-ppm limit for my resin?
No. We will review the design, confirm a supplier, and quote. The moisture target and the drying cycle come from the material supplier’s datasheet for that grade, or from a method you agree with the producing shop. We will not invent those numbers.
Send drawings for a nylon or resin-drying review
If the part is nylon, PET, PC or another hygroscopic grade, send the model or drawing, the exact material (or the datasheet), quantity, and the duty the part has to live in. We’ll review the design for manufacture, confirm which supplier would make it, and only then quote. We will not invent a drying temperature or a moisture limit for your grade.