Molded part defects usually come from one of four sources: part design, mold design, resin or processing. Knowing which helps you ask the right question when a sample arrives with sink, warp or flash. This guide describes the common injection molding defects, what they look like, their usual causes, and where the fix usually lies. It is a buyer’s guide to the conversation with your supplier, not a process-setting manual; every defect should be diagnosed on the actual tool and resin.
Defects at a glance
| Defect | What it looks like | Usual causes | Where the fix usually lies |
|---|---|---|---|
| Sink marks | Shallow depressions over thick areas, ribs or bosses | Thick sections, insufficient packing, gate freezing early | Design (core out) and process (pack/hold) |
| Voids | Bubbles inside thick sections | Same as sink, inside the part | Design and process |
| Warp | Part bends or twists out of shape | Uneven shrinkage from uneven walls, cooling or fiber orientation | Design, mold cooling, process, resin |
| Short shot | Part not completely filled | Thin walls, long flow, poor venting, low pressure | Design, gating, venting, process |
| Flash | Thin fins of plastic at parting lines or inserts | Worn or poorly fitted mold, excessive pressure, low clamp | Mold maintenance and process |
| Weld (knit) lines | Visible lines where flow fronts meet | Holes, multiple gates, flow around features | Gate location, design, process |
| Flow lines | Wavy patterns near gates | Slow or uneven flow, cold mold | Process and gate design |
| Burn marks | Black or brown marks at end of fill | Trapped air heated by compression (dieseling) | Venting and injection speed |
| Splay (silver streaks) | Silvery streaks in the flow direction | Moisture in resin, degraded material | Resin drying, temperature |
| Jetting | Snake-like patterns from the gate | Melt shooting into an open cavity | Gate design and speed |
| Ejector pin marks / stress whitening | Marks or white areas at ejector locations | High ejection force, too little draft | Draft, ejection design, cooling |
| Delamination | Surface layers peel | Contamination or incompatible material | Resin handling |
Sink marks and voids
Sink appears when the surface sets while the inside continues to shrink. Thick sections, ribs too thick for the wall, and solid bosses are the usual design causes. Processing can reduce sink with more packing pressure and time, but only while the gate stays open. If the part design has thick sections, the lasting fix is to core them out. See uniform wall thickness. For sink on cosmetic faces, including fixes in order of cost and how to write a sink requirement, see sink marks in injection molding.
Warp
Warp is uneven shrinkage. Uneven walls, uneven mold cooling and, in fiber-filled resins, fibers aligning with flow all cause parts to shrink differently in different places. Semi-crystalline resins such as PP, nylon and acetal are more prone to warp than amorphous resins. Fixes include more uniform walls, ribs placed to resist bending, better mold cooling, gate relocation and process changes. Fixtures that hold parts while cooling are a last resort. Our plastic part warpage guide matches common warp shapes to their causes and covers flatness callouts.
Short shots and flash
Short shots and flash are opposite ends of the same balance. Raising pressure to fill a thin area can force flash at the parting line. If both appear, the root cause is often design (walls too thin for the flow length) or venting and gating, not settings. Flash on an older tool often points to wear at the parting line and needs mold maintenance. Our guide to flash on injection molded parts shows how to tell tool, process and wear apart by where the flash sits.
Send samples or CAD for a defect review
Weld lines
Weld lines form wherever two flow fronts meet: around holes, between gates, behind cores. They can be weak, especially in filled resins, and visible on glossy or colored parts. They cannot always be avoided, but gate placement can move them to non-critical, hidden areas. Mold-flow simulation predicts their location before cutting steel. Ask where weld lines will fall during the DFM review. Our page on knit lines and weld lines shows how to mark cosmetic and structural zones on the drawing so the gate plan keeps them out of the way.
Splay and burn marks
Splay is usually moisture. Hygroscopic resins such as nylon, PC, PET and PBT must be dried before molding; inadequate drying causes splay and can reduce strength. Burn marks usually mean trapped air: vents are blocked or missing, or injection is too fast for venting. Both are typically processing or mold maintenance fixes.
Diagnosing a defect
Useful questions when a defect appears: Does it appear on every part or only some? In every cavity or one? At startup, after a stoppage, or steadily? Did it start after a resin lot change, a color change, a maintenance event or a process change? Is it in the same place each time? A defect that appears in one cavity points to that cavity; one that started with a new lot points to the material; one that appears in the same place on every shot from day one usually points to design or mold design. Photos with locations and lot numbers make the conversation much faster.
Defects that show up later
- Stress cracking: parts crack weeks later, often near screws, inserts or areas exposed to chemicals such as cleaners or lubricants. Molded-in stress and chemical exposure combine; PC and acrylic are especially sensitive.
- Dimensional drift: semi-crystalline resins can keep shrinking slightly after molding, and nylon changes size as it absorbs moisture. Measure parts after conditioning, not straight off the press.
- Creep and relaxation: parts under constant load deform slowly, loosening snaps and press fits.
- Color shift: UV exposure or heat aging changes color in unstabilized grades.
These are usually design and material questions rather than molding faults, but they are worth raising with the supplier before sampling.
Defects and buyers
- Define cosmetic grades and acceptable defects for each face before sampling; a limit sample or boundary sample helps.
- Ask the supplier which defects are design-driven and which are process-driven. Design issues need your decision.
- Ask for mold-flow analysis on cosmetic or warp-sensitive parts.
- Check first samples (T1) critically, but expect some adjustment; record defects with photos and locations.
- Make sure process fixes are documented so they repeat at production.
Defects in other processes, compared
| Process | Typical defects |
|---|---|
| Thermoforming | Thinning, webbing, mark-off, chill marks |
| Rotational molding | Bubbles, uneven walls, warp of flat panels |
| Vacuum casting | Bubbles, incomplete cure, mold-line marks |
| CNC machining | Tool marks, burrs, stress cracking, warp after machining |
| 3D printing | Layer lines, warp, porosity, support marks |
Ask also how the supplier will keep process changes under control once production starts. A documented process window and a first-off check after any change help stop defects from returning.
Prevention starts at design
Many molding defects are decided before the tool is built: walls, ribs, draft, gate location and the resin grade. A DFM review catches most of them. For cosmetic faces, discuss gate location, weld lines and texture early; see draft angles.
Frequently asked questions
What causes sink marks in injection molding?
Thick sections that keep shrinking after the surface sets. Coring out thick areas is the lasting fix; packing pressure helps within limits.
What causes warp?
Uneven shrinkage from uneven walls, uneven cooling or fiber orientation. Semi-crystalline resins are more prone.
Can weld lines be removed?
Not always, but gate location can move them to hidden or low-stress areas.
What causes silver streaks (splay)?
Usually moisture in the resin. Hygroscopic resins must be dried properly before molding.
Are defects the molder’s fault?